Iron–Tannin Black on Cotton Fabric: Kasim Dyeing Tests by Agrawal et al. and Ageing Tests by Wilson et al.

In accelerated thermal ageing, Wilson et al. found that their iron–tannin dyed cotton “lost tensile strength faster and more significantly than undyed equivalents” (Chemistry Central Journal, 2012). The authors note that the mix of damage mechanisms in heat ageing may differ from natural ageing. Their dye was gall and sumac tannin with iron(II) sulphate, not kasim.

Kasim is a black dye made by fermenting jaggery with scrap iron. Agrawal et al. name it as part of Kalamkari, Bagh, Ajrakh, Bagru and Mata-ni-pachedi. They write that it is “widely used for hand painting and hand block printing on textiles”. We describe that printing method in a post on hand block print kaftans. They write that kasim is applied to fabric first treated with a tannin-based mordant, usually myrobalan. Wilson et al. also put tannin on cotton first and iron second. The two papers tested different things, so each finding below stays with its own source.

How did Agrawal et al. make kasim and dye cotton cambric with it?

Agrawal et al. fermented four sugars with iron scrap, then dipped myrobalan-mordanted cotton cambric in each liquor “for a few seconds”, with no heat. The fabric was “100% cotton cambric fabric with a thread count of 210 x 215”, bought in a New Delhi market.

The four sugars were organic cane jaggery, chemically washed cane jaggery, date palm jaggery and sugarcane juice. Each jaggery was mixed with iron scrap at 1:2 (sugar to iron) In 250 ml of water. Sugarcane juice was mixed at 5:1 (ml of juice to g of iron), with no water. The liquors stood in covered glass beakers to ferment.

The fabric was scoured in 5 g/l detergent at 80 °C per 30 minuti. It was then treated with 20% owf myrobalan nut powder (Terminalia chebula) a una 1:30 sistema liquido, 70 °C, per 45 minuti. It was dried, and loose powder was brushed off by hand. After dipping in kasim, the fabric was laid on blotting paper. The colour developed within 1–2 minuti.

Samples were dyed on set days of fermentation. Each reading in Tables A and B below is one dyeing. Each reading is the average of three spots on that sample.

Does longer-fermented kasim dye cotton cambric darker? Agrawal et al.’s colour readings by fermentation day

Agrawal et al. write that K/S values “indicated a general increase as fermentation progressed”, but their own Table 2 shows the rise stopping at a peak for each sugar. K/S measures colour depth, here at 530 nm. Higher K/S means a deeper colour.

Tabella A. K/S of cotton cambric dyeings by fermentation day (Agrawal et al. 2025, Tabella 2). Bold marks each sugar’s highest value.
Day of fermentation Organic cane jaggery Chemically washed cane jaggery Date palm jaggery Sugarcane juice
1 6.02 5.2 5.95 8.12
4 10.21 11.65 9.62 15.24
7 14.32 12.1 9.45 19.05
11 17.5 12.51 11.33 18.55
14 16.33 13.37 17.6 18.28
18 15.92 13.79 17.55 17.87
21 14 16.25 11.9 18.08
26 13.63 15.19 11.16 18.91
30 13.1 15.26 10.53 18.32

Each sugar peaked on a different day. Sugarcane juice peaked first and then stayed close to its peak. Organic cane jaggery and date palm jaggery fell clearly after their peaks. Chemically washed cane jaggery peaked last and lowest, and dipped a little after its peak. So a longer ferment gave a deeper colour only up to a point, and that point depended on the sugar.

Agrawal et al. also report CIE L*a*b* values. L* runs from black to white, so a lower L* means a darker shade.

Tabella B. L* of cotton cambric dyeings by fermentation day (Agrawal et al. 2025, Tabella 3). Bold marks each sugar’s lowest (darkest) valore.
Day of fermentation Organic cane jaggery Chemically washed cane jaggery Date palm jaggery Sugarcane juice
1 35.68 38.81 41.59 31.87
4 25.66 21.12 26.84 21.87
7 19.38 22.61 23.55 17.09
11 17.81 21.90 23.18 17.32
14 19.28 22.24 19.97 18.47
18 19.89 19.45 17.63 16.06
21 21.37 18.51 24.90 15.12
26 22.19 18.97 25.32 16.08
30 22.80 19.24 25.91 15.91

L* fell steeply after the first day for all four sugars. Each then rose again after its darkest reading, most for date palm and organic cane jaggery. The darkest L* and the highest K/S did not always fall on the same day. Most a* and b* readings in the paper’s Table 3 are small, which means little red, verde, yellow or blue. The day-one date palm jaggery dyeing has the highest a* and b* in the table, so it was the reddest and yellowest. The paper describes the shades as brown-black to charcoal-black.

How did kasim-dyed cotton cambric rate for washing, sfregamento, perspiration and light in Agrawal et al.’s tests?

Agrawal et al. report that “fastness to washing, rubbing and perspiration ranged from good to excellent, while fastness to light rated poor”. The tests were ISO 105-C06 (lavaggio), ISO 105-X12 (sfregamento), ISO 105-E04 (sudore, acidic and alkaline) and ISO 105-B02 (leggero). Staining and fading use the grey scale. Light uses the blue wool scale. On both, a higher number is better. For how these scales work, vedi la nostra nota su colour bleeding and fastness.

Tabella C. Colour fastness of kasim-dyed cotton cambric, one dyeing per sugar (Agrawal et al. 2025, Tabella 4). The paper does not say on which fermentation day these dyeings were made.
Kasim fermented with Lavaggio: macchiatura da colore Lavaggio: fading Sfregamento a secco: macchiatura da colore Sfregamento a secco: fading Sfregamento a umido: macchiatura da colore Sfregamento a umido: fading Perspiration: macchiatura da colore Perspiration: fading Leggero (blue wool)
Organic cane jaggery 4-5 3-4 4 4-5 4 4-5 4-5 3-4 2-3
Chemically washed cane jaggery 4-5 3-4 4-5 4-5 4 4-5 4-5 3-4 2
Date palm jaggery 4-5 3-4 4-5 4-5 4-5 4-5 4-5 3-4 2
Sugarcane juice 4-5 3-4 4-5 4-5 4-5 4-5 4-5 3-4 2

The authors write that the dyed fabric “did not stain the adjacent undyed fabric, but it faded slightly on washing”. They conclude that the sugar source had “little or no impact” on fastness. Light fastness was the weak point for all four. Since the fermentation day of these samples is not stated, these ratings cannot be matched to a row of Table A or Table B. The paper did not test fabric strength.

Does an iron–tannin dye weaken cotton fabric before ageing? Wilson et al.’s strength, acidity and iron tests

Wilson et al. write that “the application of the dyes caused significant loss of tensile strength (breaking load) and extensibility in the textiles, even before any accelerated ageing had occurred”. Their dyes were not kasim, and their tannin was not myrobalan. Agrawal et al. did not test strength. Neither paper tells you how strong kasim-dyed cotton is.

Wilson et al. dyed woven cotton fabric on a winch and a jigger at the University of Manchester’s dyehouse. Each recipe put the cotton through a tannin bath (UN) and an iron bath (B) in turn. In these cotton recipes, the authors write, “tannic acid was the mordant”.

Table D. Wilson et al.’s dye formulations for cotton fabric (Wilson et al. 2012, Tabella 1). These are three recipes, not three dyes.
Formulation Bath A (tannin) Bath B (iron) Bath order
c1 15 g/L tannic acid, 20 °C, 2 ore 0.04 M iron(II) sulphate, 20 °C, 2 ore ABABAB
c2 15 g/L tannic acid, 20 °C, 2 ore 0.04 M iron(II) sulphate plus 0.005 M copper sulphate, 20 °C, 2 ore ABABAB
c3 16.6 g/L non-purified gall powder, 20 °C, 2 ore 0.024 M iron(II) sulphate, 20 °C, 2 ore ABABAB

The tannic acid in c1 and c2 was an even mix of non-purified Chinese gall extract and purified sumac extract.

Table E. Iron content and lightness of undyed and dyed cotton fabric (Wilson et al. 2012, Tabella 2). Standard deviations in brackets.
Misura Undyed cotton Dyed with c1 Dyed with c2 Dyed with c3
Iron, XRF ratio 15 (1) 683 (145) 742 (41) 1115 (44)
L* (lower is darker) 84.31 (0.51) 35.7 (0.91) 33.58 (0.50) 29.61 (1.01)

All three recipes put a large amount of iron into the cotton and made it much darker. The authors describe the shades as “mid to dark blue-grey”. The recipe with the most iron gave the darkest cotton. Under the microscope, iron in the cotton fibres “was easily detected on the exterior and the interior of each fibre and was most concentrated on the exterior”. In wool, per contrasto, the iron stayed mainly on the outside of the fibre.

Table F. Surface pH, breaking load and extension of unaged cotton fabric (Wilson et al. 2012, Tabella 3). Standard deviations in brackets.
Misura Undyed cotton Dyed with c1 Dyed with c2 Dyed with c3
Surface pH 6.61 (0.11) 2.72 (0.06) 2.65 (0.07) 2.48 (0.04)
Breaking load (N) 73.2 (7.7) 68.3 (5.3) 51.0 (4.8) 45.7 (8.6)
Extension (%) 10.5 (1.1) 6.9 (0.7) 9.2 (1.3) 10.2 (1.9)

Every recipe made the cotton more acidic and lowered its breaking load. Extension was lower for every recipe, but only slightly for c3. The authors suggest the damage “could be due to the acidity (pH 4 A 6)” of the dyebaths. In the same table, Wilson et al. list a black cotton Akali Sikh turban from the British Museum among their iron–tannin dyed museum objects. Its surface pH was 3.39. The paper does not give its age or dye recipe.

What happened to Wilson et al.’s iron–tannin dyed cotton fabric during accelerated ageing?

In Wilson et al.’s Table 4, the breaking load of cotton dyed with c1 fell at every weekly reading. The fabric was aged at 80 °C e 58% relative humidity, with a reading each week. Only the c1 cotton was aged; the authors chose c1 because it used the purest reagents.

Table G. Breaking load and extension of cotton fabric during accelerated ageing (Wilson et al. 2012, Tabella 4). Standard deviations in brackets.
Sample and measure At week 0 At week 1 At week 2 At week 3 At week 4
Undyed cotton, breaking load (N) 117.1 (9.2) 101.9 (15.7) 107.2 (11.6) 107.1 (8.3) 108.2 (11.0)
Cotton dyed with c1, breaking load (N) 68.3 (5.3) 29.5 (3.9) 13.0 (0.4) 7.7 (1.1) 6.2 (0.7)
Undyed cotton, extension (%) 9.1 (0.8) 8.2 (1.0) 8.2 (0.7) 8.6 (0.5) 8.1 (0.5)
Cotton dyed with c1, extension (%) 6.9 (0.7) 4.9 (0.6) 3.7 (0.6) 3.5 (0.2) 3.5 (0.2)

The undyed cotton has a higher starting breaking load in Table G than in Table F. The paper reports both values. Compare readings within one table only, never across the two.

Table H. Colour change of cotton fabric against its unaged state during accelerated ageing (Wilson et al. 2012, Tabella 4).
Week Dyed with c1: ΔE00 Dyed with c1: ΔL* Dyed with c1: Δa* Dyed with c1: Δb* Undyed cotton: ΔE00
1 7.35 −4.23 0.30 6.92 0.62
2 10.49 −4.68 1.29 10.55 1.20
3 12.15 −5.71 2.29 12.24 1.52
4 13.24 −6.72 3.02 13.22 1.82

The dyed cotton grew redder and yellower each week, but the yellow shift (Δb*) was far larger than the red shift (Δa*). The authors explain this by “the breakdown of the blue-black iron-tannate dye complex with thermal ageing”. They suggest the strength loss came from acid hydrolysis and metal-catalysed oxidation. They add that the share of each mechanism “may be different to those experienced during natural ageing”, because of the raised temperature and humidity in the chamber.

KK Fashion Exports has served buyers worldwide since 2003. Il nostro ordine minimo parte da 100 pezzi per sciarpe stampate E 200 per abiti e caftani, per stile, per colore.

Fonti

  • Agrawal, A., Aggarwal, S. and Gupta, C. (2025). “Fermenting Kasim with Diverse Sugars – A Novel Approach to an Ancient Natural Dye”. Tekstil ve Mühendis (Journal of Textiles and Engineer), 32(137), 35–43. DOI: 10.7216/teksmuh.1557325. Full text: DergiPark.
  • Wilson, H., Carr, C. and Hacke, M. (2012). “Production and validation of model iron-tannate dyed textiles for use as historic textile substitutes in stabilisation treatment studies”. Chemistry Central Journal, 6:44. DOI: 10.1186/1752-153X-6-44. Open access under CC BY 2.0: Springer.

Sviluppo di una linea di abbigliamento donna? Vedi come lavoriamo come produttore di abbigliamento femminile in India.

Visualizza i lookbook B2B → uno scorcio delle nostre ultime collezioni. Richiedi la gamma completa: più disegni su richiesta.

Le nostre fondazioni: Sadh Samaj Charitable Trust · Help and Support Foundation

WhatsApp